| PROPERTIES
|
Unit
|
Value
|
Test Method
|
| Thickness
|
mm
|
0.5
|
1.0
|
2.0
|
3.0
|
6.0
|
8.0
|
10.0
|
12.0
|
15.0
|
20.0
|
25.0
|
ASTM D-792
|
| Density
|
Kg/m3
|
30
|
30
|
30
|
30
|
30
|
30
|
30
|
30
|
30
|
30
|
30
|
ASTM D-792
|
| Cell Size
|
mm
|
0.82
|
0.82
|
0.82
|
0.82
|
0.82
|
0.82
|
0.82
|
0.82
|
0.82
|
0.82
|
0.82
|
ASTM D-3576
|
| Thermal Conductivity
|
W/m.oC
|
0.036
|
0.036
|
0.036
|
0.036
|
0.036
|
0.036
|
0.036
|
0.036
|
0.036
|
0.036
|
0.036
|
ASTM D-5930
|
| Thermal Resistance
|
m2.oC/W
|
0.013
|
0.027
|
0.055
|
0.083
|
0.166
|
0.222
|
0.277
|
0.333
|
0.416
|
0.555
|
0.694
|
ASTM C-167
|
| Tensile Strength
|
Kg/cm2
|
MD 9
|
8
|
5.4
|
5.6
|
3.8
|
3.6
|
3.67
|
4.2
|
4.5
|
4.8
|
4.9
|
ASTM D-638
|
| CD 6
|
6.4
|
3.2
|
3.2
|
2.8
|
2.7
|
2.72
|
2.05
|
2.8
|
3.1
|
3.1
|
| Elongation
|
%
|
MD 110
|
130
|
110
|
105
|
100
|
105
|
108
|
105
|
98
|
97
|
92
|
ASTM D-638
|
| CD 95
|
100
|
100
|
95
|
85
|
90
|
87
|
80
|
80
|
75
|
65
|
| Heat Dimensional Stability
|
%
|
MD 5+
|
5+
|
4+
|
3+
|
1+
|
1+
|
1+
|
0.8+
|
0.75+
|
0.51+
|
0+
|
ASTM D-6289
|
| CD 5-
|
5-
|
4-
|
3-
|
1-
|
1-
|
1-
|
0.8-
|
0.75-
|
0.51-
|
0-
|
| Water Absorption
|
mg/cm2
|
0.00157
|
0.0031
|
0.017
|
0.0267
|
0.170
|
0.37
|
0.72
|
0.93
|
0.97
|
1.2
|
1.8
|
ASTM D-570
|
| Moisture Permeability
|
g/m2.24hr
|
0.09
|
0.16
|
0.24
|
0.39
|
0.48
|
0.52
|
0.64
|
0.96
|
1.15
|
1.6
|
2.1
|
ASTM D-570
|
| Tearing Strength
|
Kg/cm
|
1.0
|
1.8
|
1.95
|
2.0
|
4.5
|
1.5
|
2.0
|
2.0
|
2.5
|
2.8
|
3.0
|
ARNON Method
|
| The Permanent Compression
Set
(100 kgf/cm2)
|
%
|
3
|
5
|
7
|
9
|
14
|
18
|
22
|
23
|
26
|
19
|
20
|
ARNON Method
|
|
|
|
|
Also See
Below
Comparison Data Sheet Between Polyethylene